This table serves as a reference for machining challenging materials. The materials are categorized by ISO material code. For each material, the table lists potential machining challenges as well as suitable tools, cutting materials, coatings, and cutting parameters. You can use the CTRL + F keys for a quick search.

MicroTurn_Werkzeugfamilien_ICONS_EN

ISO Material Properties, Problems Possible Solutions Coatings Parameters Success Stories Applications
M

Stainless Steel
(austenitic)

1.4435 ( 316L)

1.4441 ( 316LVM)


Work hardening

Long, tough chips
Difficult chip removal

  1. Very sharp cutting edge
  2. Positive tool geometry
  3. Maximum stability; prevent vibrations.
  4. Efficient cooling (high pressure)
Tool recommendations:
MTEC, MTKH, MTKO
TiAlN

Vc: 50–80 m/min
f: 0.01–0.03 mm/rev
ap: 0.02–0.10 mm

Key points:
Generates heat, work hardens and tends to form built-up edges.
 MTNN - grooving

Dental
Medical Precision mechanics
Watch


M
Stainless steel ( austenitic)

1.4301
X5 CrNi 18-10
(304)

1.4401
X5 CrNiMo 17-12-2
(316)

1.4404
X2 CrNiMo 17-12-2
(316L)

Significant work hardening. During cutting, the material hardens very quickly in localized areas. The next cut encounters a harder edge zone.

Built-up edges Welding of material to the tool cutting edge

Long, tough chips
Difficult chip evacuation

High cutting forces
High cutting edge wear

Low thermal conductivity

Heat generation in the tool

  1. Very sharp cutting edge
  2. Positive tool geometry
  3. Maximum stability; prevents vibrations.
  4. Chip breaker
  5. Select a relatively large cutting depth to reliably cut through the work-hardened edge zone from the previous cut.
  6. Efficient cooling (high pressure)
Tool recommendations:
MTEC, MTKH, MTKO, MTEF, MTEP

TiAlN
or
AlCrN (ALCRONOS)


Vc: 30–60 m/min
f: 0.01–0.03 mm/rev
ap: 0.03–0.10 mm

Key points:
Generates heat, work hardens and tends to form built-up edges.


MTEC, 1.4401
MTKH, 1.4301
MTNN, 1.4404
Aerospace
Automotive

Connectors
Dental
Hydraulic
Medical
Watch

M 1.4305
X8 CrNiS 18-9
(303)
Contains sulfur. It is the most machinable austenitic stainless steel.




S

Superalloys

Cobalt-Chromium Alloys


CoCrW

CoCr 28 Mo 6
(M64BC)


Very high cutting forces

High cutting edge wear
Extremely abrasive material. Particularly high wear on the rake face

Low thermal conductivity
Very high heat generation


  1. Very sharp cutting edge
  2. Positive tool geometry
  3. Small corner radius (0.05 to 0.1 mm)
  4. Maximum stability; minimizes vibrations.
  5. Efficient cooling (high-pressure / CO2).
  6. Maximum stability; minimizes vibration.
Tool recommendations:
MTEC, MTKH, MTKO
AlTiSiN

(TISINOS)
Vc: 15–35 m/min
f: 0.01–0.03 mm/rev
ap: 0.02–0.10 mm

Key point:
The cutting edge wears down.

Aerospace
Connector
Sensor
Watch
S

High-Performance Nickel Alloys

Inconel ( 600, 601, 602 CA, 617, 625, 690, 718, X-750, 725)

Incoloy ( 800/800H/800HT, 825, 909)

Hastelloy X

Nimonic 75, 80A

More Alloys

Extremely high toughness

High work hardening

Built-up cutting edges

Very high cutting forces

Thermal stress on the cutting edge

Extreme temperatures in the cutting zone

Notch wear

  1. Very sharp cutting edge
  2. Positive tool geometry
  3. Small corner radius (0.05 to 0.1 mm)
  4. Maximum stability; prevent vibrations.
  5. Efficient cooling (high pressure/CO2).
  6. Maximum stability; minimizes vibration.

Tool recommendations:
MTEC, MTKH, MTKO


TiAlN
or
AlCrN
or
CBN inserts
Vc: 10–35 m/min
f: 0.01–0.08 mm/rev
ap: 0.05–0.20 mm

Key point:
Generates heat and hardens.

Guidelines

SPEC Tool Sensors

MicroTurn CBN
Aerospace
Sensor Technology
S
KOVAR ( ASTM F15 FeNi29Co17)


  1. Very sharp cutting edge
  2. Positive tool geometry
  3. Small corner radius (0.05 to 0.1 mm)
  4. Maximum stability; minimizes vibrations.
  5. Efficient cooling (high-pressure/CO₂).
  6. Maximum stability; minimizes vibration.

Tool recommendations:
MTEC, MTKH, MTKO


Key points:
Low thermal conductivity. Prone to built-up edge.


Glass-to-Metal Feedthroughs (Hermetic Seals)


S Titanium

Grade 5 titanium
Grade 4 titanium

High heat at the cutting edge

Built-up edges

High tool wear

Vibrations
Elastic behavior

Chip removal


  1. Very sharp cutting edge
  2. Positive tool geometry
  3. Constant feed rate
  4. Maximum stability; avoid vibrations.
  5. Efficient cooling (high pressure/CO2).
Tool recommendations:
MTEC, MTKH, MTKO, MTEE, MTEF, MTEP
Uncoated
or
TiAlN
Vc: 40–60 m/min
f: 0.01–0.03 mm/rev
ap: 0.02–0.08 mm

Key points:
Generates heat, tends to stick to the cutting edge, and exhibits highly elastic material behavior.

MTEE, Titanium Implant

MTKH, Grade 5 Titanium, Sleeve
Dental
Medical
Watch
N
Aluminum

EN AW-7075

Al-Zn-Mg-Cu


High strength and hardness

Built-up cutting edges

Burr formation
  1. Very sharp cutting edge
  2. Positive tool geometry
Tool Recommendations:
MTEC, MTKH, MTKO, MTEF, MTEP

Uncoated
or
DLC/ta-C (MAYURA)
Vc: 80–150 m/min
f: 0.01–0.05 mm/rev
ap: 0.05–0.20 mm

Key points:
It is harder and stronger than many other aluminum alloys, yet still machinable.


MTEP Chip Breaker Aerospace
Automotive
N
Copper
Cu-ETP/2.0060
Cutting edges
Adhesion to the cutting edge

Long, tough chips

Burr formation

Surface finish
  1. Very sharp cutting edge
  2. Positive tool geometry
  3. Cutting radius 0.05–0.10 mm
Tool recommendations:
MTEC, MTKH, MTKO
DLC/ta-C (MAYURA) Vc: 80–50 m/min
f: 0.01–0.05 mm/rev
ap: 0.05–0.15 mm

Key points:
Copper is soft and ductile; it tends to produce long chips, stick to the tool, and form burrs.




N

CuBe (beryllium copper):


Built-up edges
Welding to the cutting edge

Work hardening

Health risk
Dust/aerosols containing beryllium

Surface finish

1. Very sharp cutting edge

Tool recommendations:
MTEN for hole diameter 1 mm, MTEC, MTKH, MTKO
DLC/ta-C (MAYURA)

Note:
CuBe is prone to sticking and work hardening.

Key point:
Prone to sticking and work hardening


MTNN Copper-Beryllium Connector
N
Brass (with lead)
CuZn 39 Pb 3/2.0401

Burr formation

Surface finish


  1. Very sharp cutting edge
  2. Positive tool geometry
  3. Cutting radius 0.05–0.10 mm
Tool recommendations:
Uncoated
or
DLC/ta-C (MAYURA)
Vc: 100–200 m/min
f: 0.01–0.04 mm/rev
ap: 0.05–0.20 mm


Key points:
Very good machinability and short chips. The main challenge is burr formation.




N
Brass (lead-free)
CuZn 21 Si 3/2.0402
CuZn 42/2.0332
Build-up edges

Chip control

Burr formation

Work hardening

  1. Positive rake angle
  2. Chip-breaking step
Tool Recommendations:
MTEP, MTEF - Tools with chip-breaking steps
TiAlN
or
DLC/ta-C (MAYURA)
Vc: 80–150 m/min
f: 0.01–0.05 mm/rev
ap: 0.04–0.15 mm

Note:
Creates chip pockets without proper chip control.


MTEP Chip Breaker Watch
Plumbing fixtures
H
Tool steel (>45 HRC)

1.2343
X38CrMoV5-1

1.2379
X153CrMoV12

1.2842
90MnCrV8

Very hard and brittle materials

Notch wear on the cutting edge

Sensitive to vibrations Chipping on the cutting edge


  1. Positive tool geometry
  2. Prevent vibrations
  3. Efficient cooling (high pressure/CO2).
Tool recommendations:
TiAlN
or
AlCrN (ALCRONOS)
Vc: 40–70 m/min
f: 0.01–0.03 mm/rev
ap: 0.02–0.08 mm


O
PEEK

PEEK GF30
(30% glass fiber)

PEEK CF30
(30% carbon fiber)


Heat Generation
Poor heat dissipation. Excessive cutting speed or dull cutting edges lead to overheating, smearing, and dimensional deviations.

Elasticity, deformation Springback after machining. Deformation due to heat.

Burr Formation

Long chips, woolly chips
Chips wrap around

Abrasive
Glass fibers, carbon fibers

  1. Very sharp cutting edge
  2. Positive tool geometry
  3. Relatively high feed rates rather than high spindle speed
  4. Relatively large depth of cut
  5. Efficient cooling, often with compressed air
Tool recommendations:
MTEC, MTKH, MTKO
MTEP, MTEF
UncoatedVc: 80–200 m/min
Unreinforced PEEK

Vc: 50–20 m/min
GF30 and CF30 PEEK
f: 0.01–0.03 mm/rev
ap: 0.05–0.30 mm

Key points:
Deformation caused by heat and chip removal are critical factors.


MTKH PEEKAerospace
Automotive

Dental
Medical
Chemical


O
POM

Polyoxymethylene


Heat
Deformation and dimensional deviations.

Chip removal
Chip buildup during deep drilling

Burr formation

Poor surface quality


  1. Very sharp cutting edge
  2. Positive tool geometry
  3. Efficient cooling, often with compressed air
Tool recommendations:
MTEC, MTKH, MTKO
MTEP, MTEF
Uncoated
or
DLC/ta-C (MAYURA)

Vc: 100–350 m/min
f: 0.02–0.05 mm/rev
ap: 0.05–0.15 mm

Key points:
Very good machinability. Deformation due to heat and chip removal are critical factors.



Automotive
Plant Engineering
Food industry
Mechanical Engineering
Medical

O
Technical Ceramics

Zirconia
ZrO₂

Extreme hardness
Very high tool wear

Brittleness
Chipping and spalling

Cracking

Heat generation


  1. Extremely hard cutting materials
Tool Recommendations:
Special designs

Cutting inserts made of PCD or CBN


Key points:
Extremely hard and brittle, causes high tool wear and is prone to chipping.

Watch